Potting & Insulation

Potting Compound Degassing: Air Bubbles, Mix, Cure

Air bubbles in potting compound come from mixing, wetting or cure. A symptom-first map for finding which family you have, and the checks that prove the fix.

ZIITEK Thermal Engineering Team9 min read
Cured grey potting compound in an aluminium power module housing with a trapped air bubble beside a copper winding

Where potting compound air bubbles actually come from

A void is a volume of the assembly where the design assumed solid material, and the work it was doing is now being done by air. On a high-voltage part it reduces the insulation distance between conductors and can seed partial discharge long before the part fails; inside a coil, a bubble between two turns sits where the enamel on that wire is the only insulation left. Atlas Copco's vacuum potting note says the same from the dispensing side: pockets concentrate at corners, edges and windings, where vacuum potting is often the method of choice.

RECOM's guide to potting compounds is blunt: the protection holds only if the casting is gas- and water-tight, and air inclusions can make it an unreliable barrier. Where potting forms part of the isolation barrier, safety agencies require void-free performance to be controlled in production — which is why potting compound degassing is a reliability requirement. For where a casting sits next to conformal coating, and for the rest of the cluster, start at the potting and encapsulation hub.

The question is therefore not how to remove air bubbles in potting compound, but which of three routes this one took; only one responds to vacuum degassing.

Three families, told apart by where they sit

Diagnosis starts with two observations: where the void sits, and when it first appeared.

FamilyWhere the void sitsWhen it showsFirst thing to check
Family 1 — entrained in the mixScattered evenly through the bulk; small, round, similar sizeAlready in the cup, before pouringMixing method and mix ratio
Family 2 — trapped by geometryClustered under components, inside windings, at cavity corners; irregularAt the surface right after fill, or on the first sectionFill direction, viscosity at fill, wetting time
Family 3 — born during cureThickest section, resin-to-housing interface, a shrinkage gap at a component, or a tacky contaminated interfaceHours later, after gel, or after the first thermal cycleCure schedule, exotherm, moisture, contamination

A bubble visible in the mixing cup is family 1 whatever the part looks like later; a dry patch only where compound climbed a winding is family 2; a cavity that was not there when the part went into the oven is family 3, and no amount of degassing will fix it.

Family 1 — air you mixed in

Two-part compounds entrain air the moment they are stirred, and how much depends on how you stir far more than on the compound: a flat stick kept below the surface folds in far less air than a fast circular whip. A static mixer removes the human variable but not the ratio question — a system specified by weight and measured by volume is off by the ratio of the densities, and cures soft, tacky or brittle. The guide to potting compounds for electronics covers how the chemistries differ.

Degassing then does the obvious thing: lowering the pressure above mixed material makes entrained gas expand and rise out. Master Bond's guide to minimising bubbles in mixed epoxy suggests a container 5 to 10 times the material volume, a vacuum of about 29 inHg, and a bumping technique that cycles vacuum and release several times. Kohesi Bond's void-free potting notes give 25–29 inHg, headspace of at least 5× the resin height and 3–10 minutes at full vacuum, and note that material foams to 2–6× its volume before collapsing.

Those two agree on the physics and headspace, not on hold time — which depends on viscosity, filler loading, batch depth and how fast the foam collapses. Three minutes in a 40 mm cup of 1.0 W/m·K silicone says nothing about a 150 mm drum of 3.5 W/m·K material.

Freshly mixed grey potting compound in a plastic cup, covered in fine entrained air bubbles after hand mixing

Family 2 — air the geometry keeps

This family survives perfect degassing: the compound is air-free in the pot and still leaves a dry pocket under a transformer, because the air was never in the compound — it was in the part. The mechanism is displacement. Compound entering a cavity has to push air out ahead of it, which needs a path out and enough time to wet the surfaces it passes; tight windings, gaps under large components, connector shells and deep narrow cavities each defeat one of those conditions. Master Bond's void-free bond line guidance names poor wetting and improper dispensing, and adds the remedy that matters: the material needs enough time to fill voids and displace air, which is why slower systems fill crevices better.

  1. Fill from the bottom. Nozzle at the lowest point, outlet submerged, so the level rises instead of a stream dropping through air; in a coil, the compound climbs through the winding.
  2. Give it time, and stage it. Two passes — one to wet the geometry, a short hold, then a top-up — let trapped air escape between them. Pot life is the hard limit: once viscosity climbs, the compound stops wetting and starts bridging.
  3. Lower viscosity if the data sheet allows. Warming helps wetting, but shortens pot life and accelerates cure, so measure the gain.

Shaking a filled part moves only the bubbles already leaving. Deep module housings, where the fill climbs around busbars, are the worst case — the geometry behind the potting process for battery BMS boards. Where winding or deep-cavity voids persist, vacuum potting — filling under vacuum, not degassing — is accepted practice.

Dispensing nozzle at the bottom of a machined aluminium housing, potting compound rising through a copper coil winding

Family 3 — voids born during cure

A cured part can develop cavities that were not there when it was filled. Four mechanisms produce them, and all four look like air.

Shrinkage. Every potting compound shrinks going from liquid to solid. A rigid, highly filled system has nowhere to put it except as a gap at the interface it bonded to, or a void in the thickest section. RECOM's answer is a compound soft enough to dissipate the stress, not a harder one.

Exotherm. Thick sections of fast-curing material generate heat faster than they reject it, so the centre runs hotter than the oven, curing faster and shrinking more. It is a mass problem, set by section thickness, fill temperature and, on thick parts, a staged cure — not by degassing.

Moisture from the assembly. A board that absorbed moisture releases it when the casting heats. Master Bond lists moisture contamination and gases generated during cure among the causes of voids, and recommends prebaking components to drive off moisture and step curing at low temperature so air and volatiles escape before the cure.

Cure inhibition. Some silicones will not cure against particular contaminants — sulphur-cured rubbers, some tin compounds, certain adhesive or potting residues — leaving a sticky interface that reads as a wet void. Cleanliness is not a tunable process parameter.

None improve with more vacuum; they are fixed upstream, in cure schedule, section design and incoming cleanliness.

Four potting compound degassing parameters to fix before the first batch

Four parameters belong on the process sheet before the first production batch: two are read straight off the data sheet, two get established on your own line.

ValueWhat it decidesWhere it comes from
Vacuum level the material toleratesWhether you degas at all, and how hardData sheet, or supplier confirmation for filled grades
Degas hold and bump practiceBatch time and chamber sizeTrial at your batch depth, guided by supplier practice
Preheat ceilingViscosity gain against pot-life lossData sheet: viscosity vs temperature, pot life
Pot life at your working temperatureBatch size, and how much you fill per mixData sheet, read at the temperature you actually work at

A worked example, published as a ZIITEK case study on TIS680-12AB in a UAV ESC: the 1.2 W/m·K two-part silicone — one grade in the TIS680 series, which spans 1.0 to 3.5 W/m·K over −45 to 200 °C — mixes 1:1 by weight, cures to 65 Shore OO, and lists three cure options: 24 h at 25 °C, 2 h at 70 °C or 1 h at 100 °C. Those are source-listed alternatives for that material, not evidence that every populated board tolerates each schedule; the 100 °C option is not interchangeable with room temperature in a thick casting where exotherm already matters. Validate against your own section thickness.

Cure checks that prove the batch, not the surface

The commonest false negative in potting is a part that looks cured and is not.

  • Tack-free time. Touch the surface at the interval the data sheet gives. Still tacky means an off-ratio mix, an inhibited cure or a cold part.
  • Durometer against the data sheet value. ASTM D2240 is the standard durometer method, and the sheet gives a Shore value with a tolerance; a sacrificial casting measured against it catches partial cure a tack test misses. Confirm the scale (Shore A, OO or D) first — they are not convertible by arithmetic.
  • Section and mass loss. A cut sacrificial part is the only cheap check for family-3 voids, and doubles as the wetting check for family 2. Mass loss works only where the cure emits something — condensation-cure silicone, moisture-cure polyurethane — so on an addition-cure silicone treat a witness-cup weight as a volatiles check, not a cure check.

On high-voltage parts add hipot or partial discharge on the first article and on a periodic sample. A void that survives visual and section checks often announces itself under voltage — precisely the defect the casting exists to prevent. Inspection follows the same logic: visual on every part, cross-section on the first article, X-ray or CT on high-voltage parts — with the acceptance criterion written into the drawing rather than left as "no voids".

Cut cross-section through a potted circuit board showing a void pocket trapped under the board at a component footprint

Symptom, check, action

SymptomFirst checkActionHow you know it worked
Fine bubbles throughout, all similar sizeThe mixing cup, before pouringChange mixing method; degas with bump cycles; verify headspaceNo bubbles in the cup; no scattered voids in the section
Dry pocket under a component or inside a windingFill direction and viscosity at fillBottom-up fill, staged fill, warm the part within data sheet limitsCompound visible under the component in the next section
Bubbles only at cavity cornersVenting and fill angleTilt the part, add a vent path, slow the last part of the fillCorner filled on the next three parts
Voids after cure, worst in the thickest sectionSection thickness and exothermLower fill temperature, step cure, split the pourCut section solid at the centre after cure
Surface tacky, mottled or softMix ratio by weight vs volume; contaminationRe-weigh both components; check for inhibiting residuesDurometer inside the data sheet tolerance
Random voids, worse on humid daysMoisture in the assemblyPrebake assemblies before pottingVoid rate falls and tracks the prebake, not the weather

Before you run any of it, ask whether you need vacuum degassing at all: it addresses only air entrained during mixing.

Where ZIITEK fits

ZIITEK supplies both chemistries this procedure covers: the TIS680 two-part silicone series at 1.0–3.5 W/m·K over −45 to 200 °C, and the TIE280 two-part epoxy series at 1.2–2.5 W/m·K, both UL94-V0 in our published data. Silicone suits where shrinkage stress and thermal cycling dominate; epoxy where chemical exposure and mechanical strength do. A data sheet cannot give you your own process window, though — that comes from a section-thickness check and a cure trial on the actual assembly, which is where our applications team gets involved. If you are chasing voids on a specific part, send us the drawing, the process sheet and one sectioned reject.

Share

Send it to whoever owns the thermal budget.

Application engineers at ZIITEK working on thermal interface, sealing, EMI-absorbing and heating materials for automotive, data-center and telecom customers.

Need this material for a real design?