Form-in-Place Gasketing: Process and Design Rules
How a dispensed bead becomes a seal: cure schedules, bead geometry, gland fill, material choice, and the failure modes that pass first article inspection.

What form-in-place gasketing actually is
Form-in-place gasketing is a sealing process in which an uncured elastomer is dispensed as a bead onto a flange or into a groove by a programmed machine, then cured where it sits. The cured bead is the gasket — there is no separate part to pick up, place, align or stock. Everything else in this article follows from that one difference: the seal's cross-section is created by a dispense program instead of a die, and it is fixed by the geometry of the joint it cures inside.
The acronym family around it is worth ten seconds of sorting, because much of the search traffic for this process arrives through the wrong door. FIP (form-in-place), CIPG (cured-in-place gasket) and FIPFG (formed-in-place foamed gasket) all describe the dispensed-elastomer process this article covers, with CIPG being the term many European OEM drawings use and FIPFG denoting the foamed variant, most often a two-component polyurethane. FIPG, however, is also the name the automotive industry uses for room-temperature-vulcanizing sealant applied to an oil pan or a transmission cover — a material that bonds two rigid flanges and is never expected to be a compression gasket, so a drawing that calls for an FIPG gasket is asking for that bonded joint, not for this process. If your joint is a machined aluminum housing with a lid, you want the first group. If you are resealing an engine sump, you want the second, and the design rules below do not apply.
That distinction matters more than it looks. A dispensed compression gasket is designed to be squeezed and to push back for the life of the product. An RTV flange sealant is designed to bond, cure hard against two surfaces and hold by adhesion. Both are "form in place," both are dispensed, and they fail in completely different ways.
For the material family these beads belong to — silicone foams, sponges and cushioning grades — the parent guide on silicone foam sealing materials collects the property data and the selection logic.
The four process steps that decide whether the bead seals
A form-in-place line has four variables that matter, and the capital equipment is not one of them. Surface condition, dispense geometry, cure schedule and closure force decide the outcome; the robot only repeats whatever those four allow.
Surface energy before dispense. A bead that does not wet the substrate will sit on it rather than bond to it, and a bead that has not bonded will lift at the first thermal cycle. Mold release, machining oil, mold-release residue on die-cast aluminum and the skin on a molded plastic part all lower surface energy. Plasma or corona treatment raises it, and the treatment has a shelf life measured in hours, not weeks — which is why in-line treatment beats treating a batch and stacking it.
Dispense. Parker Chomerics' dispensing guidance for form-in-place gaskets gives the rule that catches most first-run problems: the tip's inner diameter should be about six times the largest particle size of the material. Filled conductive silicones are abrasive and coarse; a tip chosen for bead width alone will clog, surge and leave a starved section that no downstream inspection catches. Tip shape matters too — tapered tips run at lower back pressure but flex, which shows up as path wander on a long bead.
Cure. Cure chemistry sets the cycle time, and cycle time is where a dispensed gasket either fits an existing line or forces a new one. GBATECH lists three cure schedules for its EF-series form-in-place EMI gaskets: 30 minutes at 150 °C, 120 minutes at 120 °C, or 24 hours at room temperature. Those three schedules are the same chemistry under different constraints — the room-temperature route exists for assemblies that cannot take oven heat, and it costs a day of work in process. UV-cure systems collapse the wait to seconds but only where the bead line can see the light.
Two-part materials add a clock nobody puts on the process sheet. Pot life sets how long the mixed material stays dispensable: a bead dispensed after the viscosity has climbed stops wetting the groove and starts bridging it. Mix ratio is not a detail either — a two-component system specified by weight and measured by volume is off by the ratio of the densities and cures soft, tacky or brittle. Shelf life and storage temperature decide whether the ratio validated in the lab is the ratio running on the line.
Closure. The last step is the one most often left to the assembly station: how far the lid travels. A dispensed bead is compressed by the mechanical stack, not by a torque spec, so the groove depth and the boss height define the squeeze. Assemble wet and the bead also bonds, which is fine until the part has to come apart for service.

Bead geometry: height, squeeze and the fill rule nobody applies
Two published rules govern a dispensed bead, and they disagree by a few points — which is the honest answer, not a mistake.
Parker recommends a bead height of about 85% of its width with 20–30% compression at closure, and advises staying below 40% in any case. VTI Vacuum Technologies' published FIP gasket dimension guideline puts the same ratio at 80%. The spread is real and it reflects material: a stiff, highly filled bead holds a taller section than a soft unfilled one, and a two-component foam collapses further before it pushes back. Treat the number as a starting ratio and confirm it with a sectioned part.
The arithmetic the process guides skip is the one that decides whether the joint closes at all: how much of the groove the cured bead fills. Parker's O-Ring Handbook, the standard reference for elastomer gland design, puts gland fill for an elastomer seal at 60% to 85% of the available groove volume, with 75% as the optimum, and at least a 10% unfilled share as a hard requirement — that unfilled share, which the handbook calls the void, is where the material goes when it expands thermally, since elastomers expand roughly ten times as much as the steel around them (ORD 5700).
That rule was written for molded O-rings, and it transfers to a dispensed bead with one correction: you control the deposited volume directly, so you can miss the target on purpose or by accident at every part.
Work it through once and the geometry stops being abstract. Dimensions below are given as width × height. Take a D-section bead 1.5 mm wide and 1.2 mm high. Approximating the section as a half-ellipse, its area is about 0.785 × 1.5 × 1.2 ≈ 1.4 mm². Set it in a groove 2.2 mm wide and 0.9 mm deep, where the closing boss stops the lid: a groove cross-section of about 1.98 mm² (per millimetre of bead length). Fill is about 1.4 ÷ 1.98 ≈ 71%, inside the band and with room to expand, and the bead is squeezed from 1.2 mm to 0.9 mm — 25% compression, inside the 20–30% rule. That pairing, fill and squeeze together, is what a working joint looks like on paper.
Change one number and it stops working. Widen the groove to 3.4 mm at the same depth and the groove section grows to about 3.06 mm²: fill falls to 46%, and the bead — still 1.5 mm wide — has an empty channel on either side to spread into. The squeeze is unchanged — the boss still closes the lid to 0.9 mm — but the groove is now nearly twice the width of the section, so the bead sits with about a millimetre of slack on either side and nothing but friction holds it where the program put it. A lid that drags as it is fitted, vibration before the bead is bonded, or internal pressure walks the section sideways; once part of it is on the flange land instead of in the groove, the lid cannot close on the boss, and the joint leaks at the first pressure test even though the bead itself was dispensed perfectly. Go the other way and set the program to lay a 2.4 mm bead, still 1.2 mm high, into the same 2.2 mm groove. Part of the section now overhangs onto the flange land instead of sitting in the groove; counting that overhang, the section is about 2.26 mm² against 1.98 mm² of groove section — 114% of what the groove can hold, with no unfilled share left where the handbook asks for at least 10%. The lid can only close by squeezing material sideways: it ends up sitting on the bead rather than on the boss, and what escapes is pushed into the housing as a ribbon that can foul a connector or bridge a creepage path. Overfill and underfill of the groove both look acceptable on a visual inspection of the open housing, which is why they survive to the leak test.
Three practical rules follow. Keep the bead centered on the groove within about ±0.2 mm, because an off-center bead fills one side first and produces a pinch point. Add material by widening the bead within the groove width, never by deepening the groove — a wider bead that still fits the groove changes fill predictably, while a deeper groove changes the squeeze. And write the groove depth and target fill percentage on the drawing, not just the bead width: the supplier dispenses to the program, but the fill is a joint property that the part designer owns.
For joints whose acceptance criterion is an ingress rating rather than a leak rate, the squeeze and groove basics sit with the IP68 sealing design rules; what changes in a dispensed bead is only the fill calculation above.

Materials: which polymer for which joint
Four material families cover almost every dispensed gasket, and the choice is driven by the joint, not by a preference for one chemistry.
| Material | Typical hardness | Typical joint | Watch out for |
|---|---|---|---|
| Cured silicone (addition-cure, one or two part) | 30–70 Shore A | electronics and EV housings, outdoor enclosures, wide temperature range | silicone oil migration onto contacts; adhesion must be primed on some plastics |
| Silicone foam, dispensed | 20–50 Shore 00 | cushioning seals, uneven flanges, vibration plus sealing | foam cell structure decides water resistance; open cell wicks |
| Polyurethane foam (two-component) | 35–80, scale not stated by the maker (ask for it — Shore A and Shore 00 are not interchangeable) | cabinet and door seals, large industrial enclosures | upper service temperature around 80 °C; UV and hydrolysis limits outdoors |
| Conductive silicone (filled) | 40–70 Shore A | EMI joints that also seal | filler costs; galvanic pairing with the housing metal |
The hardness and temperature bands above are the ranges these material classes are normally specified in, not values lifted from one datasheet; the drawing should carry the value the part needs, quoted per part.
Two properties separate these families faster than any datasheet table. The first is compression set — the percentage of deflection the material fails to recover after a defined time at temperature. Elastomers with a high set stop pushing back; Parker's handbook is blunt that a seal can still hold after 100% set if temperature and system pressure stay steady, and that the dangerous combination is high set plus shrinkage. A dispensed gasket sees that combination on any joint that cycles. Values below 5% after aging are a reasonable target for a sealing foam, and a supplier that cannot quote a set figure against a named aging cycle has not tested the property.
The second is flame rating and what it applies to. Foam and solid silicone do not reach the same rating on the same chemistry. Foam materials are rated on their own scale (HBF, HF-1) and a V-0 claim on a foam bead needs its own evidence; the mechanics of that are covered in UL 94 V-0 silicone foam sealing. For a dispensed foam gasket, one equipment maker's published data is a useful sanity check: two-component polyurethane foam at UL 94 HBF, tack-free in about five minutes, compression set under 5%, service range −60 to 80 °C, and applied bead widths of 6–20 mm (Gluestream's FIPFG data).
Where the joint has to seal and cushion at the same time, the cell structure choice matters more than the polymer: open-cell foams pass water vapor and close to nothing else, closed-cell foams seal but need more closure force. That trade-off is set out in open-cell versus closed-cell foam for gaskets.
FIP or die-cut: the decision the sales argument skips
This is the decision the process comparison usually skips. The standard sales argument for form-in-place gasketing is tooling, inventory and scrap: no die, no minimum order of a shape, no cutting waste. All true — and all irrelevant if the joint you have is better served by a die-cut part.
| Criterion | Dispensed bead wins | Die-cut part wins |
|---|---|---|
| Annual volume | low to mid volume, high mix, demand that ramps unpredictably | high, stable volume where the die amortizes and per-part converting cost falls |
| Joint geometry | complex 3D path, narrow flange, thin wall | simple outline, wide flat flange |
| Section needed | thin, 0.3–2.5 mm | thick cushioning, 3 mm and up, or multi-layer |
| Service and rework | bonded or semi-bonded; cured silicone can often be cut out and re-dispensed | part is replaceable by definition; opens for service |
| Material mix | one dispensed chemistry | foam plus conductive fabric plus dust mesh plus tape in one part |
The service column is the one that gets priced last and hurts most. A bead that cured in a groove on a joint somebody has to open for maintenance turns a five-minute field service into a scraping job. When a joint is designed to open, a die-cut gasket that lifts out is not a cheaper compromise — it is the correct answer, and no dispense program fixes it.
As a rule of thumb, four cost buckets decide the comparison and they rarely point the same way: non-recurring tooling for the die, capital and floor space for a dispense cell, per-part material (a dispensed chemistry usually costs more per kilogram than foam sheet, though a bead wastes almost none of it), and the cost of a failed joint — scrap on a dispensed line, a replaceable part on a die-cut one. At low volume the die's non-recurring cost dominates and per-part price never recovers it; at high volume it amortizes away and the per-part material and labor difference dominates instead; in between, the number that usually settles it is the rework rate.
On the die-cut side, the material breadth is the real advantage: a converter can combine silicone foam, NBR, PORON and CR foam, conductive fabric or foil, dust mesh and double-sided tape into one laminated part, which is what most enclosure designs need anyway. ZIITEK's die-cut range includes those materials cut to a customer drawing, and its Z-FOAM®800 silicone foam is the grade that typically lands in EV battery sealing and electronics enclosures: 0.06 W/m·K thermal conductivity, a UL 94 V-0 material rating, a 25% compression stress of 20–110 kPa and a compression set of 3–5% — the datasheet does not state the aging cycle behind that figure, so ask for it before you write it on a drawing. Its IP68 figure belongs to the assembled enclosure, not to the sheet. The die-cutting process for gaskets covers what the tooling side of that looks like.
A practical middle path exists and is underused: dispense the primary seal where the joint is a complex or narrow perimeter, and specify a die-cut gasket for the serviceable cover or the connector interface on the same product. The two processes are not a site-wide decision.

Conductive FIP for EMI joints
When the joint has to shield as well as seal, the filler becomes the design. A conductive form in place gasket is a filled silicone — nickel/graphite, silver/nickel, silver/aluminum or silver/copper — dispensed onto the housing and cured into an elastomer bead that grounds the joint and closes it against the environment at the same time.
Two numbers set expectations. The GBATECH EF-series is quoted at 90–110 dB from 200 MHz to 20 GHz, and its bead sections run from about 0.3 mm high by 0.3 mm wide up to 1.7 mm high by 2.5 mm wide, height listed first — small enough that the section is set by the gap you can tolerate, not by the seal force you would like. The bead profile is chosen from three standard shapes: a D-section at about 0.75:1 height-to-width, a triangular section at 1:1 for narrow flanges that need height, and a double-D at 1:1 or above when the height must exceed the width. Volume resistivity and shielding effectiveness are then verified against MIL-DTL-83528C, the specification that governs conductive gasketing material.
The joint detail that decides long-term grounding is the metal pairing. Filler and mating surface have to be galvanically compatible, or the contact resistance drifts as the interface corrodes; nickel/graphite on nickel-plated or conductive-coated housings is a safer pairing than a silver-filled bead against bare aluminum. ZIITEK's TIS®-30FIP, a nickel/graphite silicone for dispensed EMI gaskets, is quoted at 85 dB or better at 10 GHz, and above 80 dB across 200 MHz–10 GHz, with a volume resistivity of 0.04 Ω·cm or below and 2.0 W/m·K thermal conductivity — the thermal figure matters because a bead that seals and shields a power enclosure is also in the heat path.
The failure modes that pass first article inspection
Every seal failure in this list passes first article inspection, and most pass a leak test on day one. They appear at cycle 200, or after a year in the field, which is why they belong in the design review rather than the quality report.
Compression set and creep after thermal cycling. The bead is squeezed to 25%, holds, and then slowly stops pushing back. On a joint that also moves — a battery pack that swells, as covered in battery pack silicone foam sealing, or a housing that sees sun load — the seal force falls below what the ingress path needs and water finds the low-pressure line. The mechanism is set plus shrinkage; the countermeasures are a lower-set compound, more squeeze margin, or a mechanical stop that keeps the squeeze from growing with temperature. A gasket that measured 20% set in a datasheet is not evidence about cycle 300, because set is measured at one temperature for one duration.
Outgassing and siloxane migration. Silicone releases low-molecular-weight siloxane over time and under heat. In a sealed optical module that films a lens; on a gold contact it raises contact resistance; in a relay or a connector it can cause intermittent opens. The failure is not a leak, so leak testing never finds it. Where the joint sits near optics or dry contacts, ask for outgassing data on the same ASTM E595 basis used for low-outgassing thermal materials, and treat a silicone bead as a candidate for substitution rather than a default.
Adhesion loss and a starved bead. A bead that bonded at first article can debond when the interface was contaminated upstream or when plasma treatment aged out on a weekend batch. A starved bead is worse: the bead cures before the lid closes, the material does not reach the far wall, and the gap that remains is a capillary path. Both are batch-level failures, invisible on a sample, and they are why the drawing should carry a surface-preparation requirement rather than leaving it to process notes.
Overfill and bead migration. Covered in the geometry section, and worth repeating as a failure mode: a bead with no void to expand into pushes material into the housing, bridges creepage distances and can hold a lid off its boss. The part then fails an electrical safety test rather than a leak test, and the seal gets blamed for a process error.
Rework. Cured silicone can usually be cut out of a groove and re-dispensed, which is a genuine advantage in a low-yield build. Cured foam cannot — it tears, leaves residue in the groove and the surface has to be re-prepared. If a line has a meaningful rework rate, that difference belongs in the cost model.
The wrong leak test. A pressure decay test proves the joint holds differential pressure; it does not prove an IP68 rating, because an IPX8 immersion rating is set by agreement between maker and user on time and depth — IPX7 is the one fixed immersion test — and neither is inferred from a decay curve (IEC 60529). Match the test to the claim: decay for pressure integrity, tracer gas for small leaks on a sealed module, immersion for the rating itself. And test the assembly, never the material — the same bead that holds on one housing fails on another whose flange flatness differs.

What to put on the drawing before you ask for a quote
A dispensed gasket is quoted and inspected from the drawing, and most disputes come from three omissions. Put these on it:
- Bead section: width and cured height, each with a tolerance, plus the target groove fill percentage.
- Path: centerline position with a tolerance, and a note on start/stop zones — the bead at a start point is usually wider than mid-run, so give the ends more tolerance rather than demanding a uniform section the process cannot deliver.
- Material: chemistry, hardness with its scale (Shore 00 or Shore A — they are not interchangeable), flame rating against the right standard, and the compression-set limit after a defined aging cycle.
- Assembly compression: the squeeze percentage at closure and the boss height that produces it, so the mechanical stack cannot be changed without re-checking the seal.
- Acceptance: the leak test method, its parameters and its sample plan, plus any adhesion test (a peel or pull test on a witness coupon is more useful than a visual).
Values for all five are quoted per part, because bead width, groove depth and material are set by the joint. That is also why two drawings that look similar can carry very different prices.
Two numbers to fix before the first dispense
If you take one thing from this article, take the two numbers that decide whether a form-in-place gasket seals: the cured bead's fill of the groove (60–85%, optimum 75%) and the squeeze at closure (20–30%, with 40% as the ceiling). Get both right and the process is as repeatable as its advocates claim; get either wrong and no amount of dispense accuracy saves the joint.